Corrosion of additively manufactured Ti-6Al-4V for custom orthopaedic implants
File(s)
Author(s)
Tjandra, Jessica
Type
Thesis or dissertation
Abstract
Additive manufacturing (AM) of Ti-6Al-4V allows for the development of custom-shaped, patient-specific orthopaedic implants. Hollow lattice geometries, which can only be manufactured via AM, ensures that implants have similar mechanical properties to that of the surrounding bone, preventing stress shielding. Lattice structures are also beneficial for osseo-integration, ensuring mechanical stability with surrounding bone and reducing the likelihood of implant loosening.
However, the long-term mechanical properties of AM Ti-6Al-4V lattices are not well understood in a body fluid environment, with the combined effect of pores, high surface roughness and mechanical loading. It is therefore important to assess the effect of simulated body fluid (SBF) exposure on the mechanical properties of AM Ti-6Al-4V orthopaedic implants, to ensure their reliability and safety.
Initial studies exposed bulk dogbone samples to SBF for 0, 24, 72 and 168 h which were tested under tensile loading. The ductility halved with exposure to 168 h SBF, suggesting an embrittlement phenomenon due to oxygen ingress into bulk α-Ti. Additionally, AM Ti-6Al-4V lattices were tested under fatigue loading. Lattices exposed to SBF failed at up to 18% fewer cycles compared to pristine lattices.
STEM-EDS and APT were used to measure the oxygen content near the crack tip and in the bulk of specimens. STEM-EDS shows the presence of oxygen at the crack tip and ahead of the crack. APT studies show no oxygen (0.0 at.%) present in the uncorroded specimen. In specimens exposed to SBF, TiO existed as nanograins with measured oxygen content up to 40 at.%, above the solubility of oxygen in α-Ti, whereas the oxygen content in the bulk specimen was relatively low. Finally, at the crack tip region, the oxygen content was relatively high at 10 at.%. This is likely to cause the reduced fatigue lifetime in SBF-exposed samples due to oxygen embrittlement.
However, the long-term mechanical properties of AM Ti-6Al-4V lattices are not well understood in a body fluid environment, with the combined effect of pores, high surface roughness and mechanical loading. It is therefore important to assess the effect of simulated body fluid (SBF) exposure on the mechanical properties of AM Ti-6Al-4V orthopaedic implants, to ensure their reliability and safety.
Initial studies exposed bulk dogbone samples to SBF for 0, 24, 72 and 168 h which were tested under tensile loading. The ductility halved with exposure to 168 h SBF, suggesting an embrittlement phenomenon due to oxygen ingress into bulk α-Ti. Additionally, AM Ti-6Al-4V lattices were tested under fatigue loading. Lattices exposed to SBF failed at up to 18% fewer cycles compared to pristine lattices.
STEM-EDS and APT were used to measure the oxygen content near the crack tip and in the bulk of specimens. STEM-EDS shows the presence of oxygen at the crack tip and ahead of the crack. APT studies show no oxygen (0.0 at.%) present in the uncorroded specimen. In specimens exposed to SBF, TiO existed as nanograins with measured oxygen content up to 40 at.%, above the solubility of oxygen in α-Ti, whereas the oxygen content in the bulk specimen was relatively low. Finally, at the crack tip region, the oxygen content was relatively high at 10 at.%. This is likely to cause the reduced fatigue lifetime in SBF-exposed samples due to oxygen embrittlement.
Version
Open Access
Date Issued
2024-06-28
Date Awarded
2024-10-01
Copyright Statement
Creative Commons Attribution NonCommercial Licence
License URL
Advisor
Pedrazzini, Stella
Pham, Minh-son
Alabort, Enrique
Barba, Daniel
Sponsor
Engineering and Physical Sciences Research Council
Grant Number
EP/S0232059/1
Publisher Department
Materials
Publisher Institution
Imperial College London
Qualification Level
Doctoral
Qualification Name
Doctor of Philosophy (PhD)